Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Styrolution® PS 495N - PS-I - INEOS Styrolution

Material Data Center offers the following functions for Styrolution® PS 495N:
unit conversion, PDF datasheet print, comparison with other plastics, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Styrolution PS datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
제품 설명서
Styrolution® PS 495N is a high flow, high impact polystyrene with a good heat resistance and a high stiffness.
Processing/Physical Characteristics단위시험규격
ISO 데이터
용융 부피 - 흐름 속도, MVR 9.5 cm³/10min ISO 1133
온도 200 °C -
하중 5 kg -
용융 밀도 935 kg/m³ -
용융 열전도율 0.165 W/(m K) -
용융 비열용량 2290 J/(kg K) -
이형온도 88 °C -
기계적 특성단위시험규격
ISO 데이터
인장탄성률 2000 MPa ISO 527
항복강도 26 MPa ISO 527
항복변형률 1.5 % ISO 527
파단시 평균신율 40 % ISO 527
챠피 충격 강도 , +23°C N kJ/m² ISO 179/1eU
챠피 충격 강도, -30°C 130 kJ/m² ISO 179/1eU
챠피 노치드 충격 강도, +23°C 17 kJ/m² ISO 179/1eA
열적 특성단위시험규격
ISO 데이터
하중하에서의 변형온도, 1.80 MPa 85 °C ISO 75-1/-2
하중하에서의 변형온도, 0.45 MPa 89 °C ISO 75-1/-2
비카트 연화 온도, B 88.5 °C ISO 306
선형 열팽창 계수, 평행 100 E-6/K ISO 11359-1/-2
1.5mm 평균두께에서의 난연성 HB class IEC 60695-11-10
두께 H인 제품의 난연성 HB class IEC 60695-11-10
테스트 두께 3.0 mm -
전기적 특성단위시험규격
ISO 데이터
상대 유전율, 100Hz 2.5 - IEC 62631-2-1
상대 유전뮬, 1MHz 2.5 - IEC 62631-2-1
소산 인자, 100Hz 4 E-4 IEC 62631-2-1
소산 인자, 1MHz 4 E-4 IEC 62631-2-1
CTI 500 - IEC 60112
기타 특성단위시험규격
밀도 1030 kg/m³ ISO 1183
도표
점도-변형률 , Styrolution® PS 495N, PS-I, INEOS Styrolution
전단-변형률 , Styrolution® PS 495N, PS-I, INEOS Styrolution
응력-신율 , Styrolution® PS 495N, PS-I, INEOS Styrolution
시컨트탄성율-신율 , Styrolution® PS 495N, PS-I, INEOS Styrolution
비용적-온도(pvT) , Styrolution® PS 495N, PS-I, INEOS Styrolution
인장탄성율-온도 , Styrolution® PS 495N, PS-I, INEOS Styrolution
기타 정보
사E성
PROCESSING
injection molding, Melt temperature, range: 180 - 260 °C
injection molding, Melt temperature, recommended: 220 °C
injection molding, Mold temperature, range: 10 - 60 °C
injection molding, Mold temperature, recommended: 40 °C

Polystyrol 495N can be injection moulded under different conditions depending on machinery available and articles moulded. Mass temperature can be as high as 260°C. Polystyrol 495N is suitable for gas assisted injection moulding.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com